Aluminium alloy for die casting, method for manufacturing same, and die casting method
Abstract
Provided is an aluminum alloy for die casting. The aluminum alloy includes: 3-10 wt % silicon (Si); 0.1-2.0 wt % magnesium (Mg); 0.01-1.3 wt % iron (Fe); 0.01-2.0 wt % zinc (Zn); 0.01-1.5 wt % copper (Cu); 0.01-0.5 wt % manganese (Mn); 0.01-0.5 wt % chrome (Cr); 0.01 ˜ 2.0 wt % lanthanum (La); 0.01 ˜ 2.0 wt % cerium (Ce); 0.01 ˜ 2.0 wt % strontium (Sr); rest aluminum (Al); and unavoidable impurities. The aluminum alloy is improved in not only corrosion-resistance but also physical properties.
Interactive Citation Constellation Global Citation Ranking
Interactive SVG Citation Constellation renders in Rust/WebAssembly. Prior art cited: 21 · Forward citations: 0.
Claims (14 — 3 Independent, 11 Dependent)
- Claim 1Independent Claim
A die-castable aluminum alloy consisting of: 3-10 wt % silicon (Si); 0.8-1.2 wt % magnesium (Mg); 0.01-1.3 wt % iron (Fe); 0.01-2.0 wt % zinc (Zn); 0.01-1.5 wt % copper (Cu); 0.01-0.5 wt % manganese (Mn); 0.01-0.5 wt % chromium (Cr); 0.01-2.0 wt % lanthanum (La); 0.01-2.0 wt % cerium (Ce); 0.01-2.0 wt % strontium (Sr); rest aluminum (Al); and less than 0.01 wt % of unavoidable impurities.
- Claim 2Depends on #1
The die-castable aluminum alloy according to claim 1, wherein the wt % of the lanthanum (La) is 0.1-1.0 wt %.
- Claim 3Depends on #1
The die-castable aluminum alloy according to claim 1, wherein the wt % of the cerium (Ce) is 0.1-1.0 wt %.
- Claim 4Depends on #1
The die-castable aluminum alloy according to claim 1, wherein the wt % of the strontium (Sr) is 0.1-1.0 wt %.
- Claim 5Depends on #1
The die-castable aluminum alloy according to claim 1, wherein a liquidus temperature of the die-castable aluminum alloy is 580-590 ° C., and a solidus temperature of the die-castable aluminum alloy is 475-485 ° C.
- Claim 6Independent Claim
A method of manufacturing a die-castable aluminum alloy, the method comprising: manufacturing a master alloy comprising lanthanum (La), strontium (Sr), and cerium (Ce); melting silicon (Si), magnesium (Mg), iron (Fe), zinc (Zn), copper (Cu), manganese (Mn), chromium (Cr), and aluminum (Al) in a crucible; and adding the master alloy to the crucible so that the die-castable aluminum alloy consists of 3-10 wt % silicon (Si), 0.8-1.2 wt % magnesium (Mg), 0.01-1.3 wt % iron (Fe), 0.01-2.0 wt % zinc (Zn), 0.01-1.5 wt % copper (Cu), 0.01-0.5 wt % manganese (Mn), 0.01-0.5 wt % chromium (Cr), 0.01-2.0 wt % lanthanum (La), 0.01-2.0 wt % strontium (Sr), 0.01-2.0 wt % cerium (Ce), rest aluminum (Al), and less than 0.01 wt % of unavoidable impurities at percentages by weight with respect to its total weight.
- Claim 7Depends on #6
The method according to claim 6, further comprising adding a flux to the crucible.
- Claim 8Depends on #6
The method according to claim 6, wherein the master alloy comprises an Al — Sr — La — Ce quaternary master alloy.
- Claim 9Independent Claim
A die casting method comprising: melting an ingot of a die-castable aluminum alloy, which consists of 3-10 wt % silicon (Si), 0.8-1.2 wt % magnesium (Mg), 0.01-1.3 wt % iron (Fe), 0.01-2.0 wt % zinc (Zn), 0.01-1.5 wt % copper (Cu), 0.01-0.5 wt % manganese (Mn), 0.01-0.5 wt % chromium (Cr), 0.01-2.0 wt % lanthanum (La), 0.01-2.0 wt % cerium (Ce), 0.01-2.0 wt % strontium (Sr), rest aluminum (Al); and less than 0.01 wt % of unavoidable impurities, in a melting furnace; and pouring the melted die-castable aluminum alloy from the melting furnace to a sleeve; and pushing the melted die-castable aluminum alloy into a mold by a plunger at a predetermined speed and a predetermined pressure.
- Claim 10Depends on #9
The die casting method according to claim 9, wherein the melted die-castable aluminum alloy has a temperature of 660-710 ° C.
- Claim 11Depends on #9
The die casting method according to claim 9, wherein the predetermined speed is kept at 0.10-0.25 m/s and then switched to 1.95-2.5 m/s.
- Claim 12Depends on #9
The die casting method according to claim 9, wherein the predetermined pressure comprises 93-110 kgf.
- Claim 13Depends on #11
The die casting method according to claim 11, wherein the predetermined speed is switched at a position of 355-375 mm.
- Claim 14Depends on #1, #3, #4, #5, #6
An aluminum flange shaft for a washing machine, the aluminum flange shaft comprises the die-castable aluminum alloy according to any one of claim 1 or claims 3 to 6.
Technical Overview & Description
CROSS-REFERENCE TO RELATED APPLICATIONS This application is a U.S. National Stage Application, which claims the benefit under 35 U.S.C. § 371 of PCT International Patent Application No. PCT/KR2019/010776, filed Aug. 23, 2019 which claims the foreign priority benefit under 35 U.S.C. § 119 of Korean Patent Application No. 10-2018-0099452, filed Aug. 24, 2018, the contents of which are incorporated herein by reference. TECHNICAL FIELD The disclosure relates to an aluminum alloy for die casting, a manufacturing method thereof, and a die casting method. BACKGROUND ART Aluminum (Al) is alloyed with additive elements such as copper (Cu), silicon (Si), manganese (Mn), magnesium (Mg), zinc (Zn), etc. to create various kinds of alloys, and varies in characteristics depending on the kinds of alloy. The aluminum alloy may be assorted into an alloy for casting and an alloy for work according to manufacturing methods. The casting method is classified into sand casting, mold casting, high-pressure casting, die casting, and special casting. The aluminum for work may be treated to have characteristics suitable for secondary work such as roll, extrusion, forging, press, etc. The aluminum alloy for casting includes a basic Al — Si alloy, an Al — Cu alloy for improvement in mechanical properties, and an Al — Mg alloy for improvement in high corrosion-resistance characteristics, but is mostly the Al — Si alloy. The alloy for die casting is a kind of alloy for casting, but different in alloy composition from a general alloy for casting because of a different casting method from those of sand casting, mold casting, low-pressure casting, etc. The alloy for die casting is required to have characteristics of molten metal flow and low stickiness of molten metal to a die, and thus an Al — Si alloy and an Al — Si — Cu alloy excellent in such characteristics are generally used. Aluminum is alloyed to achieve various strength and corrosion-resistance characteristics, and has been developed as alt
Cited By — Indexed Forward Citations (0 of 0 total)
No indexed citing patents in this generation yet. Ingest USPTO/PatentsView bulk citation tables via patents-ingest to expand the local forward citation graph.
References Cited — Backward Prior Art (21)
Non-Patent Literature (6)
- Espacenet machine translation of CN-107858565-A retrieved on Oct. 23, 2023 (Year: 2018).
- Espacenet machine translation of KR20130032981A retrieved on Dec. 9, 2023 (Year: 2013).
- Espacenet machine translation of CN 105296818 A retrieved on Jun. 6, 2024 (Year: 2016).
- European Search Report for European Patent Application No. 19851357.4 dated Jul. 14, 2021.
- International Search Report dated Dec. 20, 2019 in International Patent Application No. PCT/KR2019/010776.
- Office Action dated Mar. 8, 2023 in Korean PatentApplication No. 10-2018-0099452