{"pub_number":"US7828893B2","doc_number":"7828893","country":"US","kind_code":"B2","patent_type":"utility","status":"active","title":"Silicon wafer and process for the heat treatment of a silicon wafer","abstract_text":"A silicon wafer having no epitaxially deposited layer or layer produced by joining to the silicon wafer, with a nitrogen concentration of 1·10 13 -8·10 14 atoms/cm 3 , an oxygen concentration of 5.2·10 17 -7.5·10 17 atoms/cm 3 , a central thickness BMD density of 3·10 8 -2·10 10 cm −3 , a cumulative length of linear slippages ≦3 cm and a cumulative area of areal slippage regions ≦7 cm 2 , the front surface having &lt;45 nitrogen-induced defects of &gt;0.13 μm LSE in the DNN channel, a layer at least 5 μm thick, in which ≦1·10 4 COPs/cm 3 with a size of ≧0.09 μm occur, and a BMD-free layer ≧5 μm thick. Such wafers may be produced by heat treating the silicon wafer, resting on a substrate holder, a specific substrate holder used depending on the wafer doping. For each holder, maximum heating rates are selected to avoid formation of slippages.","claims":[{"number":1,"text":"A process for the heat treatment of a multiplicity of silicon wafers with a diameter of at least 300 mm said process comprising resting wafers on supports selected with regard to the upper yield stress of the wafer, and at predetermined heating and cooling rate, as follows: a) for wafers having an upper yield stress of at least 0.6 MPa, measured at a temperature of 1200° C., in a vertical furnace, resting the silicon wafers during the heat treatment on substrate holders which are in the form of a continuous concentric ring with an internal diameter of at most 250 mm and an external diameter wh","independent":true}],"description":"","inventors":[{"name":"Mueller Timo","slug":"mueller-timo","country":"DE"},{"name":"Von Ammon Wilfried","slug":"von-ammon-wilfried","country":"AT"},{"name":"Daub Erich","slug":"daub-erich","country":"DE"},{"name":"Krottenthaler Peter","slug":"krottenthaler-peter","country":"DE"},{"name":"Messmann Klaus","slug":"messmann-klaus","country":"DE"},{"name":"Passek Friedrich","slug":"passek-friedrich","country":"DE"},{"name":"Wahlich Reinhold","slug":"wahlich-reinhold","country":"DE"},{"name":"Kuehhorn Arnold","slug":"kuehhorn-arnold","country":"DE"},{"name":"Studener Johannes","slug":"studener-johannes","country":"DE"}],"assignees":[{"name":"Siltronic Ag","slug":"siltronic-ag","country":"DE"}],"examiners":["Kunemund Robert M"],"cpc_codes":["A61G 13/009","A61G 2203/70","C30B 25/12","C30B 29/06","C30B 31/14","C30B 33/02","Y10T 117/1052","Y10T 117/1068"],"ipc_codes":["C30B 15/10"],"filing_date":"2006-03-22","pub_date":"2010-11-09","grant_date":"2010-11-09","priority_date":"2005-03-24","expiration_date":"2026-03-22","application_number":"US-38685506-A","family_id":"FAM-36973657","family_members":[],"citations_made":[{"pub_number":"GB2273551A","category":"APP"},{"pub_number":"EP0829559A1","category":"APP"},{"pub_number":"US5935320A","category":"APP"},{"pub_number":"US6065615A","category":"APP"},{"pub_number":"US6133121A","category":"APP"},{"pub_number":"US6197606B1","category":"SEA"},{"pub_number":"EP1081254A1","category":"APP"},{"pub_number":"EP1087042A1","category":"APP"},{"pub_number":"US6350314B1","category":"APP"},{"pub_number":"JP2003109964A","category":"APP"},{"pub_number":"US2004040632A1","category":"APP"},{"pub_number":"WO2004090967A1","category":"APP"},{"pub_number":"EP1615261A1","category":"APP"},{"pub_number":"US7037797B1","category":"SEA"},{"pub_number":"US2006278157A1","category":"SEA"}],"non_patent_literature":["A. Karoui, F. Sahtout, F. Karoui, G. A. Rozgonyi, D. Yang, Journal of Applied Physics, 96, 2004, p. 3255.","A. Karoui, G. A. Rozgonyi, Journal of Applied Physics, 96, 2004, p. 3264.","H. D. Chiou et al., Effects of Oxygen and Nitrogen on Slip in C2 Silicon Wafers, VLSI Science and Technology, ECS, Pennington, 59, 1984.","H. R. Huff, L. Fabry and S. Kishino (Eds.), Argon-Annealed 300 mm Wafers Complementing PP-Epitaxial Layers, The Electrochemical Society Proceedings vol. 2002-2, 194-201.","T. Müller et al., Modeling and Experimental Verification of the 300 mm Ar Anneal Process, Semiconductor Silicon 2002, 9th International Symposium."],"drawings_count":0,"source_id":"google_patents_public","upstream_forward_citations":0,"metrics":{"forward_citations":14,"indexed_forward_citations":14,"backward_citations":15,"npl_citations":5,"citations_per_year":0.88,"pagerank":1.8031723499298096,"citation_rank":7120356,"pagerank_rank":17132173,"velocity_rank":8229037,"family_citations":14}}